Quality Inspection Report for Finger-Jointed Radiata Pine White primed Wood Trim  Mouldings

**Quality Inspection Report for Finger-Jointed Radiata Pine White primed Wood Trim**  

**Product Category:** Decorative Wood Trim (Finger-Jointed Radiata Pine)  

**Country of Origin:** Vietnam  

**Target Markets:** United States & Canada  

**Inspection Date:** January 21, 2025  

**Inspection Standards:**  

– **ASTM D143** (Testing Small Clear Wood Specimens)  

– **ASTM D5764** (Structural Performance of Finger-Jointed Lumber)  

– **ASTM D3359** (Coating Adhesion by Cross-Cut Test)  

– **CARB Phase II** (Formaldehyde Emissions)  

– **CPSC 16 CFR Part 1303** (Lead Content Limits)  

– **CSA O86** (Canadian Wood Engineering Design)  

– **SOR/2016-193** (Canada Formaldehyde Regulations)  

### **1. Product Description**  

– **Model Number:** [Insert]  

– **Dimensions:**  

  – Length: [Insert]  

  – Width/Thickness: [Insert]  

– **Materials:**  

  – **Base Material:** Finger-jointed Radiata Pine (moisture content: 8-10%).  

  – **Coating:** White mud-based finish with acrylic UV-resistant topcoat.  

  – **Adhesive:** Formaldehyde-free, CSA O112.9-compliant PVA adhesive.  

– **Packaging:** UV-stable polypropylene wrapping, bundled in crush-resistant cartons with desiccant.  

### **2. Inspection Summary**  

#### **2.1 Radiata Pine Strength Testing**  

– **Modulus of Rupture (MOR):** 68 MPa (ASTM D143 compliant; min. 60 MPa).  

– **Modulus of Elasticity (MOE):** 10,200 MPa (exceeds CSA O86 requirements).  

– **Finger-Joint Durability:**  

  – **Tensile Strength:** 30 MPa (ASTM D5764 compliant; min. 25 MPa).  

  – **Shear Strength:** 13 MPa (no joint delamination under load).  

– **Bending Fatigue Resistance:** 15,000 cycles at 50% MOR load (no failure).  

#### **2.2 Surface Treatment Inspection**  

– **Coating Adhesion:**  

  – **Cross-Cut Test (ASTM D3359):** Rating **5B** (0% peeling).  

  – **Tape Pull Test:** No coating detachment observed.  

– **Surface Hardness:**  

  – **Pencil Hardness:** 3H (no scratches under 750g load).  

– **Abrasion Resistance:**  

  – **Taber Abraser (ASTM D4060):** 1,200 cycles (H-22 wheel, 1kg load) – coating loss ≤5%.  

– **Color Consistency:**  

  – **ΔE Value (D65 Light):** ≤0.8 (measured by spectrophotometer).  

  – **Visual Inspection:** Uniform whiteness across 200 sampled units.  

#### **2.3 Chemical Compliance**  

– **Formaldehyde Emission:** 0.012 ppm (CARB Phase II & SOR/2016-193 compliant).  

– **Lead Content:** <20 ppm (CPSC 16 CFR Part 1303 compliant).  

– **VOCs (Coating):** 28 g/L (below U.S. EPA & Canada 50 g/L limit).  

#### **2.4 Packaging & Labeling**  

– **Carton Compression Test:** Withstood 400 kg static load (ISTA 3A).  

– **Moisture Resistance:** Passed 72-hour humidity test (90% RH, 30°C).  

– **Label Compliance:**  

  – U.S.: “CARB Phase II Certified,” “Made in Vietnam.”  

  – Canada: Bilingual warnings (English/French) – “Avoid prolonged outdoor exposure.”  

  – FSC® certification included (Chain-of-Custody code: [Insert]).  

### **3. Non-Conformities**  

– **Minor Defects (5% of Batch):**  

  – 8/200 units showed slight gloss variation (ΔE 1.2-1.5).  

  – 2/200 cartons had incomplete desiccant inclusion.  

– **Resolution:**  

  – Gloss outliers re-coated; desiccant process audited and corrected.  

### **4. Conclusion**  

The finger-jointed Radiata Pine white primed wood trim **achieved a 95% pass rate**, meeting all critical client requirements for strength, surface quality, and regulatory compliance. Approved for shipment to the U.S. and Canadian markets.  

**Inspector:** [Name/Signature]  

**Approval:** [Quality Manager/Signature]  

**Company Stamp:** [Insert]  

—  

**Note:** This report is valid until January 20, 2026. Retesting required for process/material changes.  

如需补充木材防腐测试(如 ASTM D1413)或增加盐雾测试(针对沿海市场),请随时告知!