Staining in Formply,sourcing service,Laboratory testing ,inspectors,inspection checklist,quality control,quality assurance,test,buying guide ,purchasing tips ,procurement

Staining in Formply
The most common stains associated with formply are:

  1. Rust staining
  2. Tannin staining
  3. Pinking – free phenol from the phenolic surface film.
    In the writer’s experience, most staining is due to rust deposits on the deck at the time of
    pouring or iron in the aggregate. These stains appear red/brown and are often mistaken
    for tannin staining.
    Tannin staining is the result of extractives from the wood veneer leeching from the formply
    and discolouring the concrete.
    Wood species with high extractive content are much less common than in times past due
    to weight restrictions on formply sheets. These species have been mostly replaced by
    plantation pines which have a low extractive content and do not cause tannin staining. In
    the past decade, tannin staining due to wood species has become very rare.
    Pinking is caused by free phenol in the phenolic surface film.
    The excess phenol imparts a pink or pale red discolouration to the concrete. AS 6669
    requires manufacturers to test for free phenol via the alkaline resistance test. This test is
    effective in identifying excess free formaldehyde and minimises the potential for formply
    with excess free formaldehyde to be supplied to the market.